Researchers in China have traced how screen printing degrades copper-plated silicon heterojunction (HJT) solar cells and have proposed a modified screen design intended to limit that damage in production. The work, published in Solar Energy, focuses on the printing step that applies photoresist before copper plating.
Screen printing is a standard metallization route in solar cell manufacturing, but the mechanical pressure and thermal treatment involved can harm the sensitive passivating contact structures of HJT devices, raising recombination losses and lowering conversion efficiency. Copper plating is attractive because it reduces reliance on silver, so keeping the printing step from eroding cell performance matters for scaling the approach.
Why photoresist printing differs from silver paste printing
Corresponding author Lang Zhou told pv magazine that the two processes are not comparable in mechanical terms. In silver paste printing, screen openings account for only 2–5% of the total area, and an emulsion layer prevents the mesh from touching the wafer. Full-area photoresist coating, by contrast, typically uses a screen without emulsion coverage so that resist is deposited evenly across the whole wafer, meaning the mesh contacts the wafer directly and extensively on every cycle.
Measured losses over 15,000 cycles
Earlier investigations cited by the team recorded conversion efficiency falling from 26.2% to 25.7% across 15,000 consecutive printing cycles in commercial production. The loss came mainly from open-circuit voltage and fill factor, while short-circuit current density and electrical resistance stayed largely unchanged. Minority carrier lifetime degradation rose from 0.61% with a new screen to 11.0% after 15,000 cycles.
Using three-dimensional confocal microscopy, the scientists identified progressive wear of the screen mesh knuckles as the principal cause. As knuckles wear down, their contact area with the wafer grows, placing greater mechanical stress on the passivation layers beneath. Scanning electron microscopy revealed no visible surface scratches, but photoluminescence measurements confirmed higher recombination losses, pointing to damage at the amorphous silicon/crystalline silicon interface.
Trade-off between protection and coating uniformity
To address the issue, the researchers added an emulsion buffer layer to keep the mesh off the wafer surface. Six patterns were evaluated, with emulsion coverage ratios ranging from 2.9% to 16.6%. The results showed a trade-off: higher emulsion coverage reduced mechanical damage but impaired photoresist distribution. A coverage ratio of 4.7% provided the best balance, limiting minority carrier lifetime degradation to 0.41% after 10,000 printing cycles while maintaining relatively good coating uniformity.
Zhou said the findings demonstrate that a relatively simple modification to screen design can substantially mitigate printing-induced degradation, offering a practical approach to improving manufacturing reliability for copper-plated HJT cells.
Wider push toward copper metallization
The result comes as copper contacts attract growing interest as a substitute for silver in HJT cells. In April 2026, researchers at China's Nankai University reported a silver-free HJT cell with 25.2% efficiency, using plasma-induced interface engineering and copper electroplating to address adhesion, contact resistance and stability challenges at the ITO interface. Separately, scientists at Germany's Forschungszentrum Jülich reached 23.08% with a fully copper-metallized HJT cell, a relatively small penalty compared with its silver-metallized counterpart, while a version combining silver-copper paste on the front side with silver contacts on the rear reached 23.95%. Those findings underline copper's potential to cut silver consumption, although further improvements in processing and electrical performance remain necessary.