Rubber & Plastic Products

Natural Pigment Masterbatches Survive PLA and PBS Extrusion, but Light Stability Remains the Limit

A study compounds spirulina, curcumin, beetroot and chlorophyllin into PLA and PBS color masterbatches, finding most survive standard melt processing while xenon exposure still shifts their color.

Alessandra RicciNovember 2, 20265 min read0 views
Four colored polymer strands in blue, yellow, red and green leave a laboratory twin-screw extruder and enter a water bath, illustrating pigment retention during melt compounding.

Researchers have examined whether four commercial natural pigments can survive conventional melt processing in polylactic acid (PLA) and polybutylene succinate (PBS), and found that most pigment–polymer combinations can be compounded and molded on standard equipment, though color fastness under light remains the main obstacle.

The study, "Sustainability in the Development of Natural Pigment-Based Colour Masterbatches and Their Application in Biopolymers", used blue spirulina, yellow curcumin, red beetroot and green chlorophyllin. Each pigment was compounded with PLA and PBS into color masterbatches on a twin-screw extruder, then let down into the matching polymer at 2, 4 and 6 wt% and injection molded into test specimens. The masterbatch formulations also contained titanium dioxide, calcium carbonate and stearic acid, added to support UV protection, dispersion and processing.

A narrow thermal window

Heat is the central constraint. Thermogravimetric analysis put the degradation onset at approximately 229 °C for spirulina, 244 °C for curcumin, 258 °C for chlorophyllin and 267 °C for beetroot — below the degradation temperatures of the two polyesters. The researchers therefore set extrusion profiles that melted each matrix while limiting the pigments’ thermal exposure: 145 °C for PBS and 190 °C for PLA, with the twin-screw running at 65 rpm and a feed rate of 2 kg/h.

That window suited most pigment–polymer pairs but not all. Spirulina lost its characteristic blue color during PLA processing, so no blue PLA masterbatch could be produced. In PBS, whose lower processing temperature is gentler on the pigment, the same colorant compounded successfully. The result shows that pigment compatibility depends strongly on the thermal processing requirements of the matrix rather than on the colorant alone.

Flow and mechanical effects stay small

Rheology changed only modestly. Melt flow rate decreased slightly after pigment incorporation, indicating a small rise in melt viscosity; neat PLA measured about 50 g/10 min and the natural-pigment masterbatches stayed close to that value, with PBS showing a comparable minor reduction. For compounders this matters, because a color system that forces major changes to screw design, pressure settings or molding conditions offers little practical value.

Mechanical properties held within the same range across the 2 to 6 wt% additions. PLA started from a Young’s modulus of about 1710 MPa and tensile strength of 65.6 MPa, PBS from about 392 MPa and 34.5 MPa, and the colored formulations stayed near those baselines. Impact strength also remained in a similar band, although individual pigments introduced some variation.

Light exposure is the weak point

Successful extrusion did not translate into durable color. After 50 hours of xenon-lamp exposure, most formulations exceeded a color difference of ΔE* = 2, the threshold for a visually perceptible change. The exception was a PLA formulation containing 2 wt% green chlorophyllin masterbatch, which showed the highest photostability.

The study points to UV stability as the largest barrier to broader use. Packaging, consumer products, agricultural parts and outdoor applications would likely need additional stabilization, protective coatings or pigment modification before natural colors could match conventional systems over long service periods.

An environmental advantage, with caveats

Under the study’s assumptions, one kilogram of curcumin pigment generated about 0.04 kg CO2-eq, against 18.65 kg CO2-eq for the inorganic green reference pigment, and the natural-pigment masterbatches also consumed less electricity during extrusion and pelletizing.

The study concludes that natural pigment masterbatches still require development, particularly in lightfastness and thermal stability. Even so, the trials indicate that several natural colorants can be compounded into PLA and PBS on conventional equipment with only limited shifts in melt viscosity and mechanical performance, and that future work should target color stability during processing and subsequent service exposure.